Scaling out the density dependence of the $\alpha$ relaxation in glassforming polymers
Extracted source text ยท arXiv cond-mat/0404040
\documentclass{epl}
%\documentclass[showpacs,preprint,amsmath,pre]{revtex4}
\usepackage{graphicx}
%\usepackage{dcolumn}
\begin{document}
%\preprint{ }
\shorttitle{Scaling out}
\title{Scaling out the density dependence of the $\alpha$ relaxation in
glassforming polymers}
\author{C. Alba-Simionesco\inst{1}, A. Cailliaux\inst{1}, A. Alegr\`{\i}a\inst{2},
G. Tarjus\inst{3}}
\institute
{\inst{1} Laboratoire de Chimie Physique, B\^atiment 349,
Universit\'e de Paris Sud, F-91405 Orsay, France \\
\inst{2} Departamento de F\'\i\'{\i}sica de Materiales,
Facultad de Qu\'\i mica, Universidad del Pa\'\i s Vasco (UPV/EHU),
Apartado 1072, 20080 San Sebasti\'an, Spain\\
\inst{3} Laboratoire de Physique Th{\'e}orique des
Liquides, Universit{\'e} Pierre et Marie Curie, 4 Place Jussieu,75252
Paris Cedex 05, France }
\date{submitted to Europhys. Lett., March 11, 2004}
\maketitle
\begin{abstract}
We show that the density and temperature dependences of the
$\alpha$-relaxation time of several glassforming polymers can be described
through a single scaling variable $X=e(\rho)/T$, where $e(\rho)$ is well
fitted by a power law $\rho^x$, $x$ being a species-specific
parameter. This implies that ``fragility'' is an intrinsic,
density-independent property of a glassformer characterizing its super-Arrhenius
slowing down of relaxations, and it leads us to
propose a modification of the celebrated Angell plot.
\end{abstract}
\pacs{64.70.Pf, 61.20.Lc.-p, 61.44.+e}{}
%\vspace{1cm}
%\hrulefill\
%\narrowtext
\def\be{\begin{equation}}
\def\ee{\end{equation}}
\def\bea{\begin{eqnarray}}
\def\eea{\end{eqnarray}}
\def\bit{\begin{itemize}}
\def\eit{\end{itemize}}
The glass transition of liquids and polymers is conventionnally
studied at constant, usually atmospheric, pressure $(P)$ by cooling the
system. However, in an effort to disentangle the effects of density $(\rho )$
and temperature $(T)$ that both influence the viscous slowing down under
isobaric conditions and to provide a more stringent test of existing
models and theories, there has recently been an increasing number of
sytematic studies of glass formation using both $T$ and $P$
as experimentally controlled variables. Glassforming polymers
are interesting in this respect : first, because of their rather high
compressibility allowing to cover a significant range of densities and second, because
of the important role played in polymer science by the free-volume
theory that puts the emphasis on congestion effects due to the
increase of density as one approaches the glass transition\cite{ferry}.
In this letter we analyze new dielectric relaxation data obtained on
several glassforming polymers up to 3 kbars poly(epichlorhydrine)
(PECH), poly(vinylmethylether) (PVME), poly(vinylacetate) (PVAc),
poly(methylmethacrylate) (PMMA)), and a combination of dielectric, neutron scattering and calorimetric data on
1,4-poly(butadiene) (1,4-PB). We
show that the $\rho$ and $T$ dependences of the
$\alpha$-relaxation time ($\tau_\alpha$ expressed, say, in seconds) can be described by a single scaling
variable $X=e(\rho)/T$,
\begin{equation}
\label{eq1:equation}
log(\tau_\alpha(\rho,T)) = F(\frac{e(\rho)}{T}),
\end{equation}
where, over the range of densities experimentally accessible, $e(\rho)$
can be fitted by a power law, $\rho^x$; the parameter $x$ and the
function $F(X)$ are species-specific. This scaling generalizes to
polymers work recently done on several molecular liquids. As a
spin-off, we show that ``fragility'', a concept introduced by Angell\cite{angell85}
to characterize the degree of deviation from Arrhenius behavior in the
$T$-dependence of $log(\tau_\alpha)$ as one approaches the glass transition,
is independent of density and is thus an inherent property of each
glassformer. This leads us to suggest a modification of the widely
used Angell plot.
As a more extensive data base on the $P$ and $T$
dependences of the $\alpha$-relaxation time (and of the viscosity) of
glassforming polymers and liquids now becomes available\cite{schug98}, and
reasonably accurate equations of state exist to convert $P,T$ results
to $\rho,T$ results, the question arises of how to best organize the
data, in a model-free and physically meaningful manner. In the case
of molecular liquids, it has been recently suggested that the $\rho $
dependence could be described through a single parameter, an effective
activation energy $E_{\infty }(\rho)$ characteristic of the high-$T$
Arrhenius regime, i.e., $log(\tau_\alpha(\rho,T)) = F(E_{\infty }(\rho)/T)$. The
same procedure, however, is not applicable to glassforming polymers
because most of them cannot be studied at $T$ high enough for
reaching an Arrhenius regime, so that
%(because of ????)
$E_{\infty }(\rho)$ cannot be directly determined. In the cases studied in
\cite{CAS02} $E_{\infty }(\rho)$ was a quite featureless, increasing function
of $\rho$ (in the accessible range); rather than using an (uncontrolled)
extrapolation of the data at high $T$, it then seems more sensible to
choose a simple predefined function of $\rho$, $e(\rho)$, with as few
adjustable parameters as possible, to build a scaling variable
$X=e(\rho)/T$. An appealing choice is a one-parameter power law, $\rho^x$,
$x$ being material-specific. Such a choice has been used to represent
$\alpha$-relaxation time data for the fragile glassforming liquid
ortho-terphenyl (o-TP), with $x=4$\cite{toelle01}; it is also
consistent with a recent study of the density dependence of the
glass-transition line $T_g(\rho)$ of several polymers (up to few kbars),
where it was found that $T_g(\rho)\alpha\rho^x$, with $x\approx2.0$ for atactic
poly(propylene), $x\approx 2.7$ for poly(styrene), and $x\approx 3.4$ for
poly(carbonate)\cite{hollander01}. We have thus analyzed the
$\alpha$-relaxation time $\tau_\alpha(\rho,T)$, obtained from dielectric relaxation
measurements made on PECH, PVME, PVAc, and PMMA over a wide range of
$T$ and $P$ (all experimental details are given in \cite{aude03,
chauty03, Alegria}) and converted to $(\rho,T)$ via the equation of state
proposed by Sanchez and Cho \cite{PVT}, as a function of $\rho^x/T$, $x$
being an adjustable parameter. As illustrated in Fig. 1
% and 2
, a very good scaling of the
data is indeed reached. We find $x\approx 2.7$ for PECH and PVME, $x\approx 1.4$ for
PVAc, and $x\approx 1.25$ for PMMA. We have applied the same analysis to the
$\alpha$-relaxation time data obtained on 1,4-PB \cite{14PB} with $x\approx 1.8$. In
all cases a good data collapse is found with Eq. (1)
and $e(\rho)=\rho^x/T$ : see inset of Fig. 4.
\begin{figure}[t]
\centering
%
\resizebox{10cm}{!}{\includegraphics [height=6cm]{fig1.eps}}
\caption{
Scaled plot of
% the logarithm of the dielectric relaxation time
$log(\tau _\alpha (\rho ,T))$
versus $X = \rho ^x/T$ for PVME($x=2.7$) and
PVAc($x=1.4$). Data were obtained at atmospheric pressure and along different isotherms and
isobars up to 300MPa.}
%
\label{fig1}
%
\end{figure}
Before discussing some of the consequences of the scaling, it is worth
stressing that despite its appealing form, the power law behavior of
$e(\rho)$ may not convey much physical content. For o-TP it was suggested
that the $\rho^4/T$ scaling was reminiscent of the well-known scaling
property of simple liquids interacting via a soft repulsive pair
potential, $v(r)=\epsilon(\frac{\sigma}{r})^n$, with $n=12$ as in the
Lennard-Jones model\cite{Hansen}: indeed, for such systems the
long-time properties depend on $\rho $ and $T$ only through a single
combination $\rho T^{-3/n}$, hence for $n=12$, $\rho T^{-1/4}$, or
equivalently, $\rho^4/T$. However, such an interpretation implies a
strong corollary, that the excess thermodynamic properties of the
system (measured with respect to the ideal gas contribution) should
also depend on the scaling variable, $\rho T^{-3/n}$ or $\rho^{n/3}/T$,
only. We have checked that this is not the case for any of the
polymers considered here (nor for o-TP): as illustrated in Fig. 2 for
PVME and PB, the quantity $(\frac{P}{\rho T})$ obtained from the existing
equations of state is not a unique function of $\rho^x/T$ with $x$
determined from the scaling plot of the $\alpha$-relaxation time. Not
unexpectedly, in the available range of $\rho $,
polymers do not behave
as soft repulsive spheres. The power law $\rho^x$ should thus be
considered as a convenient, one-parameter way of representing the $\rho $
dependence of the activation energy scale $\propto e(\rho)$, a scale that, when
data are available at high enough $T$, can be identified with the
empirical Arrhenius activation energy $E_\infty (\rho )$
\cite{CAS02}. Actually, a good agreement to the $\alpha $-relaxation time
data can also be obtained by choosing a one-parameter linear
description, $e(\rho)=\rho -\rho ^*$ : see Fig. 3. Again, no special emphasis
should be put on the fact that $e(\rho)$ is a linear function of $\rho $;
this merely reflects the fact that over the limited range of density
that is accessible experimentally, $e(\rho)$ increases monotonically with
$\rho$ in a featureless fashion.
\begin{figure}[t]
%
\resizebox{12cm}{!}{\includegraphics{fig2.eps}}%
%
\caption{
Equation of state $P/\rho T$ versus $X=\rho ^x/T$ for PVME calculated from \cite{PVT} along isobars;
inset : 1,4-PB along two isochores.
Note the absence of scaling.}
%
\label{fig2}
%
\end{figure}
%
%
Besides the fact that it helps organizing all experimental data
obtained by changing $P$ and/or $T$ in a simple and rational way, the
main consequence of the scaling expressed by Eq.~(\ref{eq1:equation})
is that "fragility", which characterizes the super-Arrhenius
$T$-dependence of the $\tau _{\alpha } $ and the viscosity, is an intrinsic
property of a glassformer, in that it does not vary with density. The
concept of fragility has proved to be most useful in the study of
glassforming liquids and polymers and is now part of the very lexicon
of such studies. Quantifying the degree of fragility of a system can
be conveniently done without having recourse to fitting formulae by
considering the steepness index at constant density, $m_{\rho ,\tau }$,
defined as
%
\begin{figure}[t]
\centering
%
\resizebox{10cm}{!}{\includegraphics{fig3.eps}}
%
\caption{
Scaled plot $log(\tau _\alpha (\rho ,T) )$ versus $X=e(\rho )/T$ with $e(\rho )=
\rho -\rho ^*$ for PVME ($\rho ^*=0.62$) and PVAc ($\rho ^*=0.29$); same symbols as in Fig.1.}
%
\label{fig3}
%
\end{figure}
%
\begin{equation}
\label{eq2:equation}
m_{\rho ,\tau }= \frac{\partial log(\tau_\alpha)}{\partial (\frac{T_\tau }{T})}\bigg|_{\rho }(T=T_\tau ),
\end{equation}
%
where $T_\tau $ is the temperature at which $\tau _\alpha =\tau $ (expressed, say,
in sec.) at the given $\rho $. By using Eq.~(\ref{eq1:equation}) and
defining $X_\tau $ as the value of the scaling variable such that $F(X_\tau
)= log(\tau )$, it is easy to show that $m_{\rho ,\tau }=X_\tau F'(X_\tau )$, where
$F'(X_\tau )=\frac{dF(X)}{dX}$, is {\em independent of density}. Thus
fragility, when properly defined, is an intrinsic property of the
glassformer. Breakdown of this feature may occur when major structural
changes take place in the system under compression, as for instance in
tetrahedrally bonded liquids such as $SiO_2$ or $H_2O$ in which the
local coordination is known to change with density. The empirical
observation that fragility may vary with {\em pressure} is a
consequence of the possible change in the relative contributions to
slowing down due to $T$ and to $\rho $. Indeed, the steepness index at
constant pressure, $m_{P,\tau }$, defined by an equation similar to
Eq.~(\ref{eq2:equation}) is related to that at constant density
through
\begin{figure}[t]
\centering
%
\resizebox{10cm}{!}{\includegraphics{fig4.eps}}
%
\caption{
Modified Angell plot : $log(\tau _\alpha )$ versus $X/X_g$ where $X_g$ is the
glass transition value ($\tau _\alpha = 100 sec$ or $\eta = 10^{13}mPa.s$) for
all polymers shown in inset. For comparison we also show as full and
dashed lines the scaled curves for o-terphenyl and glycerol,
respectively\cite{CAS02}. Inset : scaled plot $log(\tau _\alpha (\rho , T)$
versus $X=\rho ^x/T$ for several polymers, PVME, PECH($x=2.7$),
PMMA($x=1.25$), PVAc($x=1.4$), 1,4-PB ($x=1.8$) and o-terphenyl
($x=4$).}
%
\label{fig4}
%
\end{figure}
\begin{equation}
\label{eq3:equation}
m_{P ,\tau }(P)= m_{\rho ,\tau }(1+\alpha_P/|\alpha_\tau|),
\end{equation}
%
where $\alpha_P=-\rho^{-1}(\partial \rho/\partial T)_P$ and $\alpha_\tau=-\rho^{-1}(\partial \rho/\partial T)_\tau$ are the
isobaric and isochronic coefficients of expansivity; the ratio
$\alpha_P/|\alpha_\tau|$ characterizes the relative effect of $\rho $ over that of $T$
at constant $P$ when $\tau _\alpha =\tau $\cite{ferrer98}. $(1+\alpha_P/|\alpha_\tau|)$ is
also equal to $\frac{H_P}{E_V}$\cite{naoki87}, with
$H_P=(\partial\ln(\tau_\alpha)/\partial(1/T))_P$ and $E_V=(\partial\ln(\tau_\alpha)/\partial(1/T))_\rho$). One can
see from Eq.~(\ref{eq3:equation}) that the fragility measure at
constant $P$ is always larger than the constant-$\rho $ fragility and
that its variation with $P$ depends on that of the ratio $\alpha_P/|\alpha_\tau|$;
the amplitude and the sign of this latter is species-specific : for
instance it has been shown to decrease with increasing $P$ in the case
of glycerol (resulting in a decrease of the fragility with
pressure\cite{cook94}) and to increase with $P$ in the case of
1,4-polybutadiene\cite{ferrer98}. Combining Eq.~(\ref{eq1:equation})
and
Eq.~(\ref{eq3:equation}) gives
%
%\begin{equation}
%\label{eq4:equation}
$\alpha_P/|\alpha_\tau| = \alpha _P \frac{dln (e(\rho ))}{dln(\rho) } T_\tau$,
%\end{equation}
%
%
which in the case of a power law behavior $e(\rho )=\rho ^x$ simply reduces to $\alpha _P. x .T_\tau $, where both
$\alpha _P$ and $T_\tau $ depend on $P$; usually $\alpha _P$ decreases with $P$\cite{alba91} and $T_\tau $ increases
with $P$, lead to a variety of behavior for $\alpha_P/|\alpha_\tau|$ (see above).
The fact that fragility is an intrinsic property of a glassformer is
best represented by modifying the now standard Angell
plot\cite{angell85} in which $log(\tau _\alpha )$ is shown versus the inverse
scaled temperature $T_g/T$ at constant (usually atmospheric) pressure
: we suggest instead, when enough data is available, to plot $log(\tau
_\alpha) $ versus $X/X_g$, where $X= e(\rho )/T$ is the scaling variable
introduced above and $X_g$ its value when $\tau _\alpha $ reaches a
characteristic "glass transition" value, say $\tau _\alpha = 100sec$ for
dielectric relaxation data. The steepness of the $log(\tau _\alpha
)$-vs-$X/X_g$ curve is a measure of the intrinsic fragility of a
system, since indeed, according to Eq.~(\ref{eq1:equation}),
\begin{equation}
\label{eq4:equation}
m_X= \frac{dlog(\tau _\alpha)}{d(X/X_g)}\bigg|_{X=X_g}= X_g F'(X_g),
\end{equation}
%
is equal to $m_{\rho ,\tau }$ at the chosen glass transition point. The
modified Angell plot is shown in Fig. 4 where all the polymer data
considered in this study (see inset of Fig. 4) are displayed together
with results for a "fragile" liquid o-terphenyl and an "intermediate"
one, glycerol\cite{CAS02}.
In conclusion, we have shown that the $P$ and $T$ dependences of the
$\alpha$-relaxation time of glassforming polymers and liquids can be
combined, after conversion to $\rho - T$ data, in a function of a single
scaling variable $X =e(\rho)/T$, where $e(\rho )$ is well fitted by a power
law $\rho ^x$, $x$ being species-specific. On the practical side, this
provides a simple way to organize and display the increasing amount of
isobaric and isothermal relaxation time data on glassforming polymers
and liquids. On the theoretical side, this suggests that fragility is
an intrinsic property of a glassformer, which is best illustrated on a
modified Angell plot $log(\tau _\alpha )$ versus $X/X_g$, and that $e(\rho )$
characterizes the density dependence of the "bare" activation energy
scale.
\section*{Acknowledgments} This work has been funded by the CNRS, University Paris-Sud,
University P. et M. Curie, in spite of the lack of support to
fundamental research from the present French Government.
We would like to dedicate this letter to our late coworker and friend
Daniel Kivelson whose stimulating presence and creative thinking we
miss very much.
%
\begin{thebibliography}{99}
%
\bibitem{ferry}
J.D.~Ferry, {\em "viscoelastic properties of polymers"} (Whiley, New-York, 1980);
G. B. McKenna, in Comprehensive Polymer Science {\bf 2}, vol. 2, C. Booth and C. Price
Eds. (Pergamon, Oxford 1989) p. 31.
%
\bibitem{angell85}
C.~A.~Angell,
in {\em Relaxations in Complex Systems}, K.L. Ngai and G. B. Wright Eds. (U.S.
Dept. of Commerce, Springfield, 1985), p. 3.
%
\bibitem{schug98}
K.~U.~Schug, H.~E.~King, and R.~B\"ohmer,
J. Chem. Phys. {\bf 109}, 1472 (1998);
G. Floudas, G. Fytas, T. Reisinger, G. Wegner, J. Chem.
Phys. {\bf 111}, 9129 (1999);M. Paluch, G. Gapinski, A. Patkowski and E.W. Fischer, J. Chem. Phys.
{\bf 114}, 8048 (2001); R. Casalini, C. M. Roland, J. Chem. Phys. {\bf 119}, 4052 (2003);
C.M.~Roland, R.~Casalini, P.~Santangelo, M.~Sekula, J.~Ziolo, and M.~Paluch,
Macromolecules {\bf 36}, 4954 (2003).
%
\bibitem{CAS02}
C.~Alba-Simionesco, D.~Kivelson, and G.~Tarjus,
J. Chem. Phys. {\bf 116}, 5033 (2002);
G.~Tarjus, S.~Mossa , D.~Kivelson, and , C.~Alba-Simionesco J. Chem. Phys. march (2004).
%
\bibitem{toelle01}
A.~T\"olle, Rep. Prog. Phys. {\bf 64}, 1473 (2001);
%\bibitem{dreyfus03}
C.~Dreyfus, A.~Aouadi, G.~Gapinski, M.~Matos-Lopez, W.~Steffen,
A.~Patkowki, and R.~M.~Pick, Phys. Rev. E, {\bf 68}, 011204 (2003).
%
\bibitem{hollander01}
A.~G.~S.~Hollander and K.~O.~Prins,
J. Non-Cryst. Solids {\bf 286}, 1 (2001).
%
\bibitem{aude03}
A.~Chauty-Cailliaux, C.~Alba-Simionesco, D. Gomez, and A. ~Alegria,
submitted (2004);
A.~Alegria, C.~Elizetxea, I.~Cendoya, and J.~Colmenero,
Macromolecules, {\bf 28}, 8813 (1995).
%
\bibitem{chauty03}
A.~Chauty-Caillaux, PhD Thesis university Paris-Sud, Orsay, july 2003.
%
\bibitem{Alegria}
A.~Alegria and D. Gomez unpublished results; D. Gomez, PhD thesis,
Universidad del Pa\'is Vasco, San Sebasti\'an, dec 2001.
%
\bibitem{PVT}
I.C.~Sanchez and J.~Cho,
Polymer {\bf 36}, 2929 (1995).
%
\bibitem{14PB}
B.~Frick, C.~Alba-Simionesco,K.H.~Andersen and L.~Willner,
Phys. Rev. E {\bf 67}, 051801(2003);
A.~Chauty-Cailliaux, C.~Alba-Simionesco, B.~Frick, I.~Goncharenko, L.~Willner,
Phys.Rev.E rapid Comm {\bf 67}, 010802 (2003).
%
\bibitem{Hansen}
J.~P.~Hansen and J~.~R.~Mc Donald,
{\em Theory of Simple Liquids}, (Academic Press Limited, London, 1986).
%
\bibitem{ferrer98}
M.~L.~Ferrer, C.~Lawrence, B.~G.~Demirjian, D.~Kivelson, G.~Tarjus,
and C.~Alba-Simionesco, J. Chem. Phys. {\bf 109}, 8010 (1998);
G.~Tarjus, C.~Alba-Simionesco, M.~L.~Ferrer, H.~Sakai, and D.~Kivelson,
in {\em ``Slow Dynamics in Complex Systems''},
M. Tokuyama and I.~Oppenheim Eds.
(ACS Books, Washington, 1999), p. 406.
%
\bibitem{naoki87}
M.~Naoki, H.~Endou, and K.~Matsumoto,
J. Chem. Phys. {\bf 91}, 4169 (1987).
%
\bibitem{cook94}
R.~L.~Cook, H.~E.~King Jr., C.~A.~Herbst, and D.~R.~Herschbach,
J. Chem. Phys. {\bf 100}, 5178 (1994).
%
\bibitem{alba91}
C.~Alba-Simionesco in
{\em Hydrogen-Bonded Liquids}, J. Dore and J. Teixeira Eds, NATO ASI, Kluwer, 1991),
p. 81.
\end{thebibliography}
%
%
\end{document}